MP159 is an alloy of the Multiphase family of alloys possessing the unique combination of ultra-high strength, ductility and corrosion resistance. Through work strengthening and aging, MP159 alloy exhibits ultimate tensile strength levels in excess of 265,000 psi while maintaining reduction of area values greater than 30%. Excellent strength and ductility are also evident at elevated temperatures up to 1100 – 1200 °F. Additionally, the alloy displays exceptional corrosion resistance and resistance to crevice and stress corrosion in various hostile environments. MP159 alloy is produced by vacuum induction melting followed by VAC-ARC remelting (VIM-VAR) to provide optimum control of chemistry and preferred ingot solidification.
Weight % | Ni | Co | Cr | Fe | Mo | Ti | Cb | Al |
---|---|---|---|---|---|---|---|---|
Typical Composition | 25.5 | 35.7 | 19.0 | 9.0 | 7.0 | 3.0 | 0.6 | 0.2 |
Characteristics | English | Metric | |
---|---|---|---|
Nominal density | 77°F / 25°C | 0.301 lbs/in3 | 8.33 gr/cm3 |
Coefficient of thermal
expansion – Linear |
77°F – 212°F
25°C – 100°C |
7.94 µ × in/in- °F | 14.3 µ × m/m- °K |
77°F – 392°F
25°C – 200°C |
7.90 µ × in/in- °F | 14.2 µ × m/m- °K | |
77°F – 572°F
25°C – 300°C |
7.88 µ × in/in- °F | 14.2 µ × m/m- °K | |
77°F – 752°F
25°C – 400°C |
8.09 µ × in/in- °F | 14.6 µ × m/m- °K | |
77°F – 932°F
25°C – 500°C |
8.28 µ × in/in- °F | 14.9 µ × m/m- °K | |
77°F – 1112°F
25°C – 600°C |
8.38 µ × in/in- °F | 15.1 µ × m/m- °K | |
77°F – 1292°F
25°C – 700°C |
8.90 µ × in/in- °F | 16.0 µ × m/m- °K | |
77°F – 1472°F
25°C – 800°C |
10.13 µ × in/in- °F | 18.2 µ × m/m- °K | |
Magnetic permeability | 77°F / 25°C | 1.00265 |
Heat Treatment | Tensile | |||||
---|---|---|---|---|---|---|
Ultimate | Yield | Elongation | Reduction
of area |
|||
KSI | MPa | KSI | MPa | % | % | |
Annealed 1925°F / 1052°C, 4 hrs, WQ | 123 | 850 | 58 | 400 | 60 | 69 |
Cold Worked 48% | 230 | 1585 | 205 | 1415 | 12 | 46 |
Cold Worked 48% + 1225°F (663°C)/ 4 hrs / AC | 275 | 1895 | 265 | 1825 | 8 | 35 |