Nickel Alloy 201

  • Nickel Alloy 201
  • General Characteristics

    Nickel 201 is the low-carbon version of Nickel 200. Typical applications are caustic evaporators, combustion boats, platter bars and electronic components. Nickel 201, because of its low base hardness and lower work-hardening rate, is particularly suited for spinning and cold forming. It is preferred to Nickel 200 for applications involving exposure to temperatures above 600°F (315°C).

  • Typical Chemical Composition

    Weight % Ni (+Co) Cu Fe Mn C Si S
    Typical Composition 99.00 min 0.25 max 0.40 max 0.35 max 0.02 max 0.35 max 0.01 max
  • Physical Properties

    Characteristics English Metric
    Nominal density 20°C   /   68°F 0.321 lbs/in3 8.89 g/cm3
    Melting range 2615-2635 °F 1435-1445 °C
    Specific heat 25°C   /   78°F 0.109 BTU/lb – °F 456 J/KG- °K
    Average coefficient of

    thermal expansion

    100°C  /  148°F 7.3 micro in/in- °F 13.2 micro m/m- °K
    200°C  /  328°F 7.7 micro in/in- °F 13.9 micro m/m- °K
    300°C  /  508°F 8.0 micro in/in- °F 14.4 micro m/m- °K
    400°C  /  688°F 8.3 micro in/in- °F 14.9 micro m/m- °K
    Thermal conductivity 100°C  /  148°F 42.4 BTU/ft- hr – °F 73.4 W/m – °K
    200°C  /  328°F 38.3 BTU/ft- hr – °F 66.3 W/m – °K
    300°C  /  508°F 34.6 BTU/ft- hr – °F 59.9 W/m – °K
    400°C  /  688°F 32.4 BTU/ft- hr – °F 56.1 W/m – °K
    Electrical resistivity 20°C   /   68°F 95 nΩ ∙ m
    200°C /  328°F 175 nΩ ∙ m
    400°C /  688°F 330 nΩ ∙ m
    600°C / 1048°F 405 nΩ ∙ m
  • Mechanical Properties

    Form Tensile
    Ultimate Yield Elongation in 50 mm (2 in.)
    Wire, cold drawn KSI MPa KSI MPa %
    Annealed 55-75 380-520 15-30 105-210 55-40
    No. 1 temper 55-100 380-690 20-80 140-550 55-35
    Spring temper 55-80 380-550 15-40 105-275 60-40
  • Specifications

    • DIN – 17753

View full Quality Metals catalogue