The 6063 alloy is a medium strength alloy commonly referred to as an architectural alloy particularly for window frames, door frames and roofs. It is normally used in intricate extrusions. It has a good surface finish, high corrosion resistance, is readily suited to welding and can be easily anodized. Most commonly available as T6 temper and in the T4 condition it has good formability.
Other | |||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|
Weight % | Si | Fe | Cu | Mn | Mg | Cr | Zn | Ti | Each | Total | Aluminum |
minimum | 0.20 | — | — | — | 0.45 | — | — | — | — | — | Remainder |
maximum | 0.60 | 0.35 | 0.10 | 0.1 | 0.90 | 0.10 | 0.10 | 0.10 | 0.05 | 0.15 |
Characteristics | English | Metric | |
---|---|---|---|
Nominal density
(68°F/20°C) |
0.097 lbs/in3 | 2.68 mg/m3 | |
Melting range | 1140°F-1210°F | 616°C-654°C | |
Specific heat
(212 °F/100°C) |
0.215 BTU/lb – °F | 900 J/KG- °K | |
Coefficient of thermal expansion | Linear
68°F – 212°F 20°C – 100°C |
12.1 micro in/in- °F | 21.8 micro m/m- °K |
Thermal conductivity
(68°F/20°C) |
0 temper | 126 BTU/ft- hr – °F | 218 W/m – °K |
T5 | 121 BTU/ft- hr – °F | 209 W/m – °K | |
T6 | 116 BTU/ft- hr – °F | 200 W/m – °K | |
Electrical conductivity
(68°F/20°C) |
Equal Volume | 0 temper | 58% IACS |
T5 | 55% IACS | ||
T6 | 53% IACS |
Temper | Tensile (0.500″ Dia. Specimen) | Hardness | Shear | Fatigue | Modulus | |||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
Ultimate | Yield | Elongation/4D | Brinell
500 kg 10 mm |
Ultimate shearing
strength |
Endurance limit-R.R.Moore type | Modulus of elasticity | ||||||
KSI | MPa | KSI | MPa | % | KSI | MPa | KSI | MPa | KSIx103 | Gpa | ||
O | 13 | 90 | 7 | 50 | 18 | 25 | 10 | 70 | 8 | 55 | 10.0 | 69 |
T4 | 25 | 170 | 13 | 90 | 22 | — | — | — | — | — | 10.0 | 69 |
T5 | 27 | 185 | 21 | 145 | 12 | 60 | 17 | 115 | 10 | 70 | 10.0 | 69 |
T6 | 35 | 240 | 31 | 215 | 12 | 73 | 22 | 150 | 10 | 70 | 10.0 | 69 |